本鋼寬板坯超低碳鋼頭坯夾雜原因分析與控制措施

  • 打印
  • 收藏
收藏成功


打開(kāi)文本圖片集

摘 要:介紹本鋼寬厚板坯冷軋超低碳鋼頭坯夾雜的形態(tài)及來(lái)源特征,針對(duì)主要影響澆次頭坯夾雜物的實(shí)際情況,分析頭坯卷渣夾雜的形成原因及影響因素,提出相應(yīng)操作和工藝改進(jìn)措施,使超低碳鋼頭坯夾雜問(wèn)題得到一定的改善。

關(guān)鍵詞:超低碳鋼;寬板坯;成因;改進(jìn)措施

THE ANALYSIS AND CONTROL MEASURES ON ULTRA LOW CARBON HEAD INCLUSION OF WIDE SLAB IN BENXI STEEL

Wang Quanzhou Xue Changjiang Yang Kuoming

(Steelmaking Plant of Bensteel Group Corporation Limited. Benxi 117000,China)

Abstract:The article introduces the morphology and source characteristics of inclusions in cold-rolled ultra-low carbon steel billets of wide and thick plates at Benxi Iron and Steel. Based on the actual situation that mainly affects the inclusions in the billets during casting, the formation reasons and influencing factors of slag inclusions in the billets are analyzed, and corresponding operational and process improvement measures are proposed to improve the problem of inclusions in ultra-low carbon steel billets to a certain extent.

Key words: ultra low carbon;wide slab;inclusion;improve measure

0 前 言

自本鋼煉鋼廠寬板坯連鑄機(jī)成立以來(lái),冷軋超低碳鋼一直是7號(hào)連鑄機(jī)重點(diǎn)生產(chǎn)品種,冷軋鋼卷表面夾雜是困擾產(chǎn)品質(zhì)量的主要技術(shù)難題之一。(剩余3630字)